Studies of natural rubber /montmorillonite nanocomposites

 

Arun Kumar, Pratibha Singh, Vishal Verma, K. N. Pandey, Vijai Kumar.

Central Institute of Plastics Engineering and Technology, Lucknow, India

. *Corresponding Author E-mail: arun7003cipet@gmail.com

ABSTRACT:

In the present work, an attempt has been made to make natural rubber/clay nanocomposite and to study the performance of nanocomposite in terms of mechanical, swelling resistance and thermal properties. The incorporation of organomodified clay has been varied from 1 phr to 7 phr in natural rubber matrix. It has been found that at 5 phr loading of organomodified clay in natural rubber matrix has shown highest tensile strength. Moreover swelling resistance of nanocomposite has drastically decreased with increasing organomodified clay loading. It has also been demonstrated by TGA analysis that thermal stability of nanocomposite has maximum thermal stability at 5 phr loading of organomodified clay. The microstructure and dispersion of the composite was investigated by scanning electron microscopy (SEM). The optimum rate of organoclay incorporation was 5 parts per hundred rubbers.

 

KEYWORDS: Natural rubber, MMT, Solution blending, tensile strength, TGA, SEM.

 


 

1. INTRODUCTION:

Natural rubber reinforced with organoclay is expected to provide products with excellent properties such as tensile strength, heat resistance, aging resistance and impermeability [1-3]. The most vital consideration in rubber/organoclay nanocomposite is the dispersion of organically modified clay particles in the rubber matrix. It is very well documented in the literature that generally three types of composites materials are obtained with the use of OMC as filler: conventional composite, intercalated nanocomposite and exfoliated nanocomposites. The exfoliated clay is the best option in term of polymer reinforcement [1,3,4]. Exfoliated clay improves the gas barrier properties and swelling resistance of the composite compared to the pristine polymer. [1-3, 5-7]. It is fact that fully exfoliated rubber/clay nanocomposite are very difficult to produce [4]. Commercial application of these polymer products have been tried where such as barrier properties are required as food and bewarwge, packaging materials. The soft rubbery materials have been used for various engineering products containing highly compressed air such as tires inner tube air spring; cure bladders etc, because of their characteristic elastic behaviour [8]. In the present study nanocomposites composed of natural rubber reinforced with modified organoclay (MMT) have been prepared by solution method and their characterization have been carried out using thermo gravimetric analyzer (TGA), differential scanning calorimetry (DSC) and scanning electron microscopy (SEM).

 

2. EXPERIMENTAL: 

2.1 Materials               

Montmorillonite clay surface modified with 15-35 wt % octadecylamine and 0.5-5 wt % aminopropyltriethoxysilane was kindly provided by sigma Aldrich, New Delhi. Natural rubber (SMR CV 60) from Polysar, Canada. Toluene was used to dissolve the rubber.

 

2.2 Preparation of nanocomposite

For preparing the NR/clay, 16g of natural rubber (SMR CV 60) were dissolved in 500 ml toluene in 1000 ml beaker. Various amount of modified clay, 1, 3, 5 and 7 phr was dispersed in 50 ml toluene. The modified-clay solution was then added to the rubber toluene solution .The solution was stirred vigorously with 30 rpm for at least 12 hours. When the solution had mixed homogenously it was removed from the beaker and was put in a Petrydish for casting. Sample was put in an open atmosphere until the solvent was evaporated. The sample was ready to analyzing.

 

3. TESTING

Density is carried out according to ASTM (792) .In this test the specimens are weight in air and then weighted suspended in solvent. The obtained values are applied in the following equation.

 

Density of material= weight of material in air/ (weight of material in air-weight of body suspended in solvent) * density of solvent.

 

For an ASTM D471-98 standard swelling test sample were immersed in a closed container filled with engine oil for 24 h. Solution content was determined by using the following equation.

                Mt [%] = wt - w0 \ w0 * 100

Where, mt, wt and w0 are the solution content at a given time, weight of the sample at the time of the measurement and initial weight respectively.

 

Tensile strength and tensile modulus of the samples were measured according to ASTM D412-2000 standard using a Universal Testing Machine, INSTRON, model no. 3382, UK and the hardness (shore A, ASTM D2240-86) was measured by hardness tester (DIN-53505). TGA were measured on a pyris TGA-1(Perkin Elmer) at 100c/min, temperature range from room temperature to 6000c .

 

The crystallization and glass transition temperature (tg) of the composite sample were studies by DSC using a Perkin Elmer Pyris Diamond, DSC in a nitrogen atmosphere in the heating and cooling rate of 20°C/minute. In the first heating and cooling scan, the sample were heated from -80  to 25°C, held at that temperature for 1 min to eliminate previous thermal history. Morphology of composite were studied by scanning electron microscopy.

 

4. RESULT AND DISCUSSION

4.1. Density of nanocomposite

It is well known fact density is a praticle phenomenon. Because of this reason as we increase the content of MMT nanofller in rubber matrix, there is a sharp increase in density. This has been shown in figure 1 and table 1.

   

Figure 1. Density of NR/clay nanocomposite with different loading of clay.

 

Table 1.  Density of NR/clay nanocomposite     

Organoclay loading (phr)

Density(g/cm3)

0

0.91

1

0.92

3

0.93

5

0.94

7

0.95

 

4.2 Swelling property of nanocomposite

The percentage of swelling a non polar solvent such as engine oil is reduced by the incorporation of MMT nanosize filler into the NR matrix. This has been shown in figure 2and table 2. This decline nature in swelling resistance may be attributed to the increase in the weight of the nanocomposite.  

 

Figure 2.  Percentage of swelling by NR/clay nanocomposite with different loading of clay.

 

Table 2. Swelling properties of NR/clay nanocomposites

Organoclay loading(Phr)

Swelling Resistance (%)

0

179

1

103

3

92

5

67

7

52

 

4.3 Effect of organoclay on mechanical properties

Table 3, Figure 3 to 6, shows values of mechanical properties of the nanocomposite with different content of MMT incorporated. In general there was a positive correlation between mechanical properties values and the quantity of MMT in the nanocomposite. Optimum values of mechanical properties are obtained at 5 phr MMT. However, at a rate of higher than 5 phr, it is evident mechanical properties do not improve and follow a decline nature. The enhancement of mechanical properties up to 5 phr MMT may be attributed to the nanometric dispersion of silicate layers in the rubber matrix. The silicate layers may favour the formation of immobilized or partially immobilized polymer phases which also increase the mechanical properties. It is also possible that the orientation of silicate layer is responsible for the observed reinforcing effect. Nanosize filler with high aspect ratio such as MMT present the advantage of high interface area between filler and rubber matrix. Actually, the strength of NR/MMT interface of the present system is responsible for increasing the modulus by increasing the MMT content. This suggests the presence of strong interaction between two kinds of substances and part of network structure in the material [9]. In this case the MMT acts as a physical cross linking junction. The reason is that the exfoliated MMT layers interact with co-polymer chains to form a physical cross linking. The tensile strength and the tensile modulus of nanocomposite also improved by nanodispersed MMT. However, when the loading amount of MMT overpasses 5 phr, the tensile strength and tensile modulus of nanocomposite does not rise and elongation at break significantly decreases. This may be because of two reasons. Firstly, the introduction of more MMT layers strongly impedes the stress- induced crystallization of pure NR. Secondly, higher MMT content easily causes the increase of the dispersion phase (non-exfoliated structure) and size of the nanocomposite prepared by solution methods [10-11].   

   

Figure 3.Tensile strength of NR/clay nanocomposite with different loading of  clay

 

Figure 4.Tensile modulus of NR/clay nanocomposite with different loading of  clay

 

Figure 5. Elongation at break of NR/clay nanocomposite with different loading of  clay

 

Figure 6. Hardness of NR/clay nanocomposite with different loading of  clay

 

Table 3. Mechanical properties of NR/clay nanocomposite

Organoclay loading (phr)

0

1

3

5

7

Tensile Strength (Mpa)

7.10

8.00

8.90

10.30

7.62

Tensile Modulus (Mpa)

2.25

2.71

2.93

2.95

2.86

Elongation at Break(%)

924

974

1174

1189

1141

Hardness

63

64

66

67

65

 

4.4. Thermal Stability of nanocomposite

The TGA thermograms of NR and its nanocomposite in nitrogen environment are depicted in figure 7 and the initial degradation temperature of the nanocomposites are summarised in table 4. The degradation rate of nanocomposite is slower than the neat natural rubber at the beginning, thereafter, the weight loss is slowed down compared to the neat NR and the exfoliated stage is more affective. It indicates that the nanocomposite has higher thermal stability than the neat NR. Enhance thermal stability of nanocomposites can be co-related to homogenous nanoclay silicate layer dispersion and to a strong interfacial adhesion between nanoclay/rubber [12]. These results show that the exfoliation of the silicate layers in rubber matrix has bestowed remarkable effect in the nanocomposite mainly in the barrier effect [13].

 

Table 4.  Initial degradation temperature obtained from TGA for NR and its nanocomposites

MMT content (%)

Initial degradation temperature (oc)

0

240 oc

1

260 oc

3

267 oc

5

375 oc

 

Figure 7.   TGA curve (relatively weight loss as a function of temperature) under N2     flow for NR/clay

 

Table 5. The glass transition temperature obtained from DSC for NR/MMT nanocomposites

MMT content (%)

Initial degradation temperature (oc)

0

- 43.0  oc

1

- 42.4  oc

3

- 41.6  oc

5

- 40.8 oc

 

DSC results are shown in figure 8 and summarized in table 5. The glass transition temperature for natural rubber compound is obtained to be - 43oc and while for nanocomposites with 1,3 and 5 phr MMT it increases to - 42.4oc,- 41.6oc and -40.8oc respectively. The natural rubber/MMT nanocomposites show a higher glass transition temperature and lower peak value suggesting a strong adhesion between NR and silicate layers [14-15].

 

 

Figure 8.   DSC curve (relatively heat flow as a function of temperature) under N2 flow for NR/clay

 

4.5. Morphology of nanocomposite

The SEM images depict that the nanocomposite having 5 phr nanoclay MMT is more dispersed than the other nanocomposites containing 1, 3 and 7 phr nanoclay MMT (figure 9). These finding are in good agreement with TGA and DSC results. Thus we can say that less than 5 phr loading of nanoclay MMT in rubber matrix offers the best properties in terms of tensile strength, tensile modulus, hardness and thermal stability.

 

  

(a)

 

 

 (b)

                                                                                                                                                Fig.(b)

(c)

 

 

(d)

  

Figure 9. SEM micrograph of NR/clay nanocomposite with different loading of MMT: fig.(a)1 phr, fig. (b) 3 phr, fig.(c) 5 phr and fig. (d) 7 phr    

 

5. CONCLUSION:

Nanocomposite from natural rubber and organomodified MMT could be prepared using solution method. With organomodified MMT, the optimum rate of organoclay incorporation is 5 phr. SEM micrographs gave a clue for better dispersion of organomodified MMT at 5 phr loading in rubber matrix. TGA result demonstrate that nanocomposite is highly stable at 5 phr loading of organoclay in polymer matrix. It has also been found that incorporation of 5 phr organomodified MMT gave maximum mechanical properties.

 

6. REFERENCES:

1.        Alexandra, p. Dubios, Mater, sci. eng. 2000, 28, 1.

2.        T.J. Pinnavaia, G.W. Beall, polymer clay nanocomposites, john willey and son, new York 2000.

3.        S. S. Ray, M. Okamota, prog. Polm. Sci. 2003,28,1539.

4.        J. Karger-Kocsis, C.- M. Wu, polym. Eng. Sci. 2004,44,1083.

5.        Y.-P.Wu, Q.-X. Jia, D.-S. Yu, L.-Q. Zhang, L.-Q. Zhang, j. Appl. polym. sci. 2003,89,3855.

6.        Z.-F. Wang, B.Wang, N.Qi, H.-F.Zhang, L.-Q. Zhang, polymer 2005, 46, 719.

7.        C. Nah, H. J. Ryu, W.D. Kim, S.-S.Choi, polym. Adv. Technol. 2002, 13, 649.  

8.        Zhang L.Q, Wang Y.Q., Sui Y, and Yu D.S. (2000) morphology and mechanical properties of clay rubber nanocomposites. Journal of Applied Polymer Science 78(11), 1873-1878.

9.        Huang J, Zhang L, effect of NCO/OH molar ratio on structure and properties of graft- interpenetrating polymer networks from polyurethane and nitrolignin, polymer, 43,2287-2294,2002. 

10.     Wu YP, Zhang LQ, Wang YQ, Liang Y, Yu DS, structure of carboxylated acrylonitrlle-butadiene Rubber (CNBR)-clay nanocomposites by coagulation rubber latex and clay aqueous suspension. J appl polym Sci, 82, 2842-2848, 2001.

11.     Valadares L.F., Leito C.AP., and Galembeck F. prepration of natural rubber montmorillonite nanocomposites in aqueous medium; evidence for polymer–platelet adhesion, polymer 47, 672-678, 2006.

12.     [Avella, M. J. Bondioli, F.Canillo,V, Pace, E. D. Errico, M. E. , Ferrari, A. M. ,Focher, B. and Malinconico, M. Poly (e-caprolactone)-based nanocomposites: influence of compatibilazation on properties of poly (e- caprolactone)-silica nanocomposites. Composite science and technology, 66, 886-894, 2006.

13.     Qin h, SU Q, Zhang s, Zhao B, Yang M. Thermal stability and flammability of polyamide 66/montmorillonite nanocomposites. Polymer, 44, 7533-7538, 2003.

14.     Varghese S, Karger-kocsis J, natural rubber based nanocomposites by latex compounding with layered silicates, polymer, 44,4921-4927, 2003. 

15.     Wang Y, Zhang H, Wu y, Yang J Zhang L, Preparation and properties of natural rubber/rectonite nanocomposites, Eur Poly J, 14, 2776 -2783, 2005

 

 

 

 

Received on 18.05.2012         Modified on 25.05.2012

Accepted on 31.05.2012         © AJRC All right reserved

Asian J. Research Chem. 5(5): May 2012; Page 623-627